Metric UnitsUS Customary Units

Mechanical Properties

Elastic (Young's, Tensile) Modulus, GPa 190
110
Elongation at Break, % 25 to 27
13
Poisson's Ratio 0.29
0.34
Shear Modulus, GPa 72
40
Tensile Strength: Ultimate (UTS), MPa 500 to 570
260
Tensile Strength: Yield (Proof), MPa 230 to 310
120

Thermal Properties

Latent Heat of Fusion, J/g 250
190
Maximum Temperature: Mechanical, °C 400
160
Melting Completion (Liquidus), °C 1450 to 1460
980
Melting Onset (Solidus), °C 1410
900
Specific Heat Capacity, J/kg-K 470
370
Thermal Conductivity, W/m-K 49 to 52
71
Thermal Expansion, µm/m-K 12
19

Electrical Properties

Electrical Conductivity: Equal Volume, % IACS 7.1 to 7.2
15
Electrical Conductivity: Equal Weight (Specific), % IACS 8.2 to 8.3
15

Otherwise Unclassified Properties

Base Metal Price, % relative 1.8
31
Density, g/cm3 7.8
8.9
Embodied Carbon, kg CO2/kg material 1.4
3.1
Embodied Energy, MJ/kg 18
51
Embodied Water, L/kg 45
350

Common Calculations

Resilience: Ultimate (Unit Rupture Work), MJ/m3 110 to 120
27
Resilience: Unit (Modulus of Resilience), kJ/m3 140 to 250
67
Stiffness to Weight: Axial, points 13
6.7
Stiffness to Weight: Bending, points 24
18
Strength to Weight: Axial, points 18 to 20
8.1
Strength to Weight: Bending, points 18 to 20
10
Thermal Diffusivity, mm2/s 13 to 14
22
Thermal Shock Resistance, points 16 to 18
9.3