ASTM A27 cast steel belongs to the iron alloys classification, while C77100 nickel silver belongs to the copper alloys. There are 26 material properties with values for both materials. Properties with values for just one material (4, in this case) are not shown.

For each property being compared, the top bar is ASTM A27 cast steel and the bottom bar is C77100 nickel silver.

Metric UnitsUS Customary Units

Mechanical Properties

Elastic (Young's, Tensile) Modulus, GPa 190
110
Poisson's Ratio 0.29
0.31
Shear Modulus, GPa 73
45
Tensile Strength: Ultimate (UTS), MPa 460 to 550
600
Tensile Strength: Yield (Proof), MPa 230 to 310
540

Thermal Properties

Latent Heat of Fusion, J/g 250
180
Maximum Temperature: Mechanical, °C 400
150
Melting Completion (Liquidus), °C 1460
990
Melting Onset (Solidus), °C 1420
950
Specific Heat Capacity, J/kg-K 470
390
Thermal Conductivity, W/m-K 52
40
Thermal Expansion, µm/m-K 12
20

Electrical Properties

Electrical Conductivity: Equal Volume, % IACS 7.0 to 7.1
7.6
Electrical Conductivity: Equal Weight (Specific), % IACS 8.1
8.5

Otherwise Unclassified Properties

Base Metal Price, % relative 1.8
27
Density, g/cm3 7.8
8.1
Embodied Carbon, kg CO2/kg material 1.4
3.5
Embodied Energy, MJ/kg 18
56
Embodied Water, L/kg 45 to 46
310

Common Calculations

Resilience: Unit (Modulus of Resilience), kJ/m3 140 to 260
1280
Stiffness to Weight: Axial, points 13
7.8
Stiffness to Weight: Bending, points 24
20
Strength to Weight: Axial, points 16 to 20
21
Strength to Weight: Bending, points 17 to 19
20
Thermal Diffusivity, mm2/s 14
13
Thermal Shock Resistance, points 15 to 18
19