MakeItFrom.com
Menu (ESC)

ASTM B541 Gold vs. ASTM A216 Cast Steel

ASTM B541 gold belongs to the otherwise unclassified metals classification, while ASTM A216 cast steel belongs to the iron alloys. There are 21 material properties with values for both materials. Properties with values for just one material (11, in this case) are not shown. Please note that the two materials have significantly dissimilar densities. This means that additional care is required when interpreting the data, because some material properties are based on units of mass, while others are based on units of area or volume.

For each property being compared, the top bar is ASTM B541 gold and the bottom bar is ASTM A216 cast steel.

Metric UnitsUS Customary Units

Mechanical Properties

Elastic (Young's, Tensile) Modulus, GPa 110
190
Elongation at Break, % 6.0 to 14
25 to 27
Poisson's Ratio 0.4
0.29
Shear Modulus, GPa 38
72
Tensile Strength: Ultimate (UTS), MPa 670 to 1180
500 to 570
Tensile Strength: Yield (Proof), MPa 480 to 900
230 to 310

Thermal Properties

Latent Heat of Fusion, J/g 90
250
Melting Completion (Liquidus), °C 1110
1450 to 1460
Melting Onset (Solidus), °C 930
1410
Specific Heat Capacity, J/kg-K 170
470
Thermal Expansion, µm/m-K 13
12

Electrical Properties

Electrical Conductivity: Equal Volume, % IACS 7.7 to 12
7.1 to 7.2
Electrical Conductivity: Equal Weight (Specific), % IACS 4.0 to 6.2
8.2 to 8.3

Otherwise Unclassified Properties

Density, g/cm3 17
7.8

Common Calculations

Resilience: Ultimate (Unit Rupture Work), MJ/m3 65 to 91
110 to 120
Resilience: Unit (Modulus of Resilience), kJ/m3 1090 to 3830
140 to 250
Stiffness to Weight: Axial, points 3.4
13
Stiffness to Weight: Bending, points 9.0
24
Strength to Weight: Axial, points 11 to 19
18 to 20
Strength to Weight: Bending, points 9.8 to 14
18 to 20
Thermal Shock Resistance, points 36 to 63
16 to 18