EN 1.5026 Steel vs. K94200 Alloy
Both EN 1.5026 steel and K94200 alloy are iron alloys. There are 17 material properties with values for both materials. Properties with values for just one material (14, in this case) are not shown.
For each property being compared, the top bar is EN 1.5026 steel and the bottom bar is K94200 alloy.
Metric UnitsUS Customary Units
Mechanical Properties
Elastic (Young's, Tensile) Modulus, GPa | 190 | |
140 |
Poisson's Ratio | 0.29 | |
0.34 |
Shear Modulus, GPa | 72 | |
54 |
Tensile Strength: Ultimate (UTS), MPa | 660 to 1980 | |
500 to 710 |
Thermal Properties
Melting Onset (Solidus), °C | 1390 | |
1440 |
Specific Heat Capacity, J/kg-K | 480 | |
500 |
Thermal Conductivity, W/m-K | 47 | |
15 |
Thermal Expansion, µm/m-K | 13 | |
5.0 |
Electrical Properties
Electrical Conductivity: Equal Volume, % IACS | 7.3 | |
2.7 |
Electrical Conductivity: Equal Weight (Specific), % IACS | 8.5 | |
3.0 |
Otherwise Unclassified Properties
Density, g/cm3 | 7.7 | |
8.2 |
Common Calculations
Stiffness to Weight: Axial, points | 13 | |
9.8 |
Stiffness to Weight: Bending, points | 25 | |
21 |
Strength to Weight: Axial, points | 24 to 71 | |
17 to 24 |
Strength to Weight: Bending, points | 22 to 45 | |
17 to 22 |
Thermal Diffusivity, mm2/s | 13 | |
3.7 |
Thermal Shock Resistance, points | 20 to 60 | |
49 to 70 |