EV31A magnesium belongs to the magnesium alloys classification, while C75400 nickel silver belongs to the copper alloys. There are 23 material properties with values for both materials. Properties with values for just one material (12, in this case) are not shown. Please note that the two materials have significantly dissimilar densities. This means that additional care is required when interpreting the data, because some material properties are based on units of mass, while others are based on units of area or volume.

For each property being compared, the top bar is EV31A magnesium and the bottom bar is C75400 nickel silver.

Metric UnitsUS Customary Units

Mechanical Properties

Elastic (Young's, Tensile) Modulus, GPa 44
120
Elongation at Break, % 3.5
2.0 to 43
Poisson's Ratio 0.27
0.32
Shear Modulus, GPa 17
46
Shear Strength, MPa 170
250 to 370
Tensile Strength: Ultimate (UTS), MPa 260
370 to 630
Tensile Strength: Yield (Proof), MPa 170
130 to 590

Thermal Properties

Maximum Temperature: Mechanical, °C 200
190
Melting Onset (Solidus), °C 590
1040
Specific Heat Capacity, J/kg-K 1000
390
Thermal Conductivity, W/m-K 86
36
Thermal Expansion, µm/m-K 27
18

Electrical Properties

Electrical Conductivity: Equal Volume, % IACS 18
7.0
Electrical Conductivity: Equal Weight (Specific), % IACS 90
7.4

Otherwise Unclassified Properties

Density, g/cm3 1.8
8.5

Common Calculations

Resilience: Ultimate (Unit Rupture Work), MJ/m3 8.1
12 to 120
Resilience: Unit (Modulus of Resilience), kJ/m3 330
75 to 1450
Stiffness to Weight: Axial, points 13
7.9
Stiffness to Weight: Bending, points 65
19
Strength to Weight: Axial, points 40
12 to 21
Strength to Weight: Bending, points 50
13 to 19
Thermal Diffusivity, mm2/s 47
11
Thermal Shock Resistance, points 16
12 to 21