Nickel beryllium 360 belongs to the nickel alloys classification, while B390.0 aluminum belongs to the aluminum alloys. There are 23 material properties with values for both materials. Properties with values for just one material (7, in this case) are not shown. Please note that the two materials have significantly dissimilar densities. This means that additional care is required when interpreting the data, because some material properties are based on units of mass, while others are based on units of area or volume.

For each property being compared, the top bar is nickel beryllium 360 and the bottom bar is B390.0 aluminum.

Metric UnitsUS Customary Units

Mechanical Properties

Elastic (Young's, Tensile) Modulus, GPa 200
76
Elongation at Break, % 1.0 to 30
0.88
Fatigue Strength, MPa 260 to 710
170
Poisson's Ratio 0.3
0.33
Shear Modulus, GPa 77
29
Tensile Strength: Ultimate (UTS), MPa 780 to 1860
320
Tensile Strength: Yield (Proof), MPa 380 to 1590
250

Thermal Properties

Melting Completion (Liquidus), °C 1330
580
Melting Onset (Solidus), °C 1200
580
Specific Heat Capacity, J/kg-K 460
880
Thermal Conductivity, W/m-K 48
130
Thermal Expansion, µm/m-K 14
20

Electrical Properties

Electrical Conductivity: Equal Volume, % IACS 5.0
27
Electrical Conductivity: Equal Weight (Specific), % IACS 5.4
88

Otherwise Unclassified Properties

Density, g/cm3 8.3
2.8

Common Calculations

Resilience: Ultimate (Unit Rupture Work), MJ/m3 12 to 190
2.6
Resilience: Unit (Modulus of Resilience), kJ/m3 360 to 3440
410
Stiffness to Weight: Axial, points 13
15
Stiffness to Weight: Bending, points 24
51
Strength to Weight: Axial, points 26 to 62
32
Strength to Weight: Bending, points 23 to 41
38
Thermal Diffusivity, mm2/s 13
55
Thermal Shock Resistance, points 19 to 46
15