SAE-AISI 4340 Steel vs. ASTM A225 Steel
Both SAE-AISI 4340 steel and ASTM A225 steel are iron alloys.
For each property being compared, the top bar is SAE-AISI 4340 steel and the bottom bar is ASTM A225 steel.
Metric UnitsUS Customary Units
Mechanical Properties
Brinell Hardness | 210 to 360 | |
190 to 250 |
Elastic (Young's, Tensile) Modulus, GPa | 190 | |
190 |
Elongation at Break, % | 12 to 22 | |
21 to 23 |
Fatigue Strength, MPa | 330 to 740 | |
330 to 390 |
Poisson's Ratio | 0.29 | |
0.29 |
Shear Modulus, GPa | 73 | |
73 |
Shear Strength, MPa | 430 to 770 | |
390 to 520 |
Tensile Strength: Ultimate (UTS), MPa | 690 to 1280 | |
620 to 830 |
Tensile Strength: Yield (Proof), MPa | 470 to 1150 | |
460 to 550 |
Thermal Properties
Latent Heat of Fusion, J/g | 250 | |
250 |
Maximum Temperature: Mechanical, °C | 430 | |
400 |
Melting Completion (Liquidus), °C | 1460 | |
1460 |
Melting Onset (Solidus), °C | 1420 | |
1420 |
Specific Heat Capacity, J/kg-K | 470 | |
470 |
Thermal Conductivity, W/m-K | 44 | |
52 |
Thermal Expansion, µm/m-K | 13 | |
13 |
Electrical Properties
Electrical Conductivity: Equal Volume, % IACS | 7.5 | |
7.3 |
Electrical Conductivity: Equal Weight (Specific), % IACS | 8.6 | |
8.4 |
Otherwise Unclassified Properties
Base Metal Price, % relative | 3.5 | |
2.3 |
Density, g/cm3 | 7.8 | |
7.8 |
Embodied Carbon, kg CO2/kg material | 1.7 | |
1.8 |
Embodied Energy, MJ/kg | 22 | |
24 to 25 |
Embodied Water, L/kg | 53 | |
48 |
Common Calculations
Resilience: Ultimate (Unit Rupture Work), MJ/m3 | 79 to 170 | |
120 to 170 |
Resilience: Unit (Modulus of Resilience), kJ/m3 | 590 to 3490 | |
580 to 820 |
Stiffness to Weight: Axial, points | 13 | |
13 |
Stiffness to Weight: Bending, points | 24 | |
24 |
Strength to Weight: Axial, points | 24 to 45 | |
22 to 29 |
Strength to Weight: Bending, points | 22 to 33 | |
21 to 25 |
Thermal Diffusivity, mm2/s | 12 | |
14 |
Thermal Shock Resistance, points | 20 to 38 | |
18 to 24 |