SAE-AISI D2 Steel vs. ASTM A27 Cast Steel
Both SAE-AISI D2 steel and ASTM A27 cast steel are iron alloys. There are 28 material properties with values for both materials. Properties with values for just one material (4, in this case) are not shown.
For each property being compared, the top bar is SAE-AISI D2 steel and the bottom bar is ASTM A27 cast steel.
Metric UnitsUS Customary Units
Mechanical Properties
Elastic (Young's, Tensile) Modulus, GPa | 190 | |
190 |
Elongation at Break, % | 5.0 to 16 | |
25 to 27 |
Fatigue Strength, MPa | 310 to 860 | |
170 to 230 |
Poisson's Ratio | 0.28 | |
0.29 |
Shear Modulus, GPa | 75 | |
73 |
Tensile Strength: Ultimate (UTS), MPa | 760 to 2000 | |
460 to 550 |
Tensile Strength: Yield (Proof), MPa | 470 to 1510 | |
230 to 310 |
Thermal Properties
Latent Heat of Fusion, J/g | 270 | |
250 |
Melting Completion (Liquidus), °C | 1440 | |
1460 |
Melting Onset (Solidus), °C | 1390 | |
1420 |
Specific Heat Capacity, J/kg-K | 480 | |
470 |
Thermal Conductivity, W/m-K | 31 | |
52 |
Thermal Expansion, µm/m-K | 11 | |
12 |
Electrical Properties
Electrical Conductivity: Equal Volume, % IACS | 4.3 | |
7.0 to 7.1 |
Electrical Conductivity: Equal Weight (Specific), % IACS | 5.1 | |
8.1 |
Otherwise Unclassified Properties
Base Metal Price, % relative | 8.0 | |
1.8 |
Density, g/cm3 | 7.7 | |
7.8 |
Embodied Carbon, kg CO2/kg material | 3.4 | |
1.4 |
Embodied Energy, MJ/kg | 50 | |
18 |
Embodied Water, L/kg | 100 | |
45 to 46 |
Common Calculations
Resilience: Ultimate (Unit Rupture Work), MJ/m3 | 92 to 100 | |
96 to 120 |
Resilience: Unit (Modulus of Resilience), kJ/m3 | 570 to 5940 | |
140 to 260 |
Stiffness to Weight: Axial, points | 14 | |
13 |
Stiffness to Weight: Bending, points | 25 | |
24 |
Strength to Weight: Axial, points | 27 to 72 | |
16 to 20 |
Strength to Weight: Bending, points | 24 to 46 | |
17 to 19 |
Thermal Diffusivity, mm2/s | 8.3 | |
14 |
Thermal Shock Resistance, points | 25 to 67 | |
15 to 18 |