C60800 Bronze vs. C75700 Nickel Silver

Both C60800 bronze and C75700 nickel silver are copper alloys. They have 65% of their average alloy composition in common.

For each property being compared, the top bar is C60800 bronze and the bottom bar is C75700 nickel silver.

Metric UnitsUS Customary Units

Mechanical Properties

Elastic (Young's, Tensile) Modulus, GPa 110
120
Elongation at Break, % 55
3.2 to 22
Poisson's Ratio 0.34
0.32
Shear Modulus, GPa 46
45
Shear Strength, MPa 290
350 to 370
Tensile Strength: Ultimate (UTS), MPa 390
590 to 610
Tensile Strength: Yield (Proof), MPa 150
470 to 580

Thermal Properties

Latent Heat of Fusion, J/g 220
200
Maximum Temperature: Mechanical, °C 210
180
Melting Completion (Liquidus), °C 1060
1040
Melting Onset (Solidus), °C 1050
990
Specific Heat Capacity, J/kg-K 410
390
Thermal Conductivity, W/m-K 80
40
Thermal Expansion, µm/m-K 18
16

Electrical Properties

Electrical Conductivity: Equal Volume, % IACS 17
8.0
Electrical Conductivity: Equal Weight (Specific), % IACS 18
8.6

Otherwise Unclassified Properties

Base Metal Price, % relative 29
30
Density, g/cm3 8.6
8.4
Embodied Carbon, kg CO2/kg material 2.9
3.6
Embodied Energy, MJ/kg 48
56
Embodied Water, L/kg 360
310

Common Calculations

Resilience: Ultimate (Unit Rupture Work), MJ/m3 170
19 to 120
Resilience: Unit (Modulus of Resilience), kJ/m3 94
930 to 1410
Stiffness to Weight: Axial, points 7.3
7.8
Stiffness to Weight: Bending, points 19
19
Strength to Weight: Axial, points 13
19 to 20
Strength to Weight: Bending, points 14
19
Thermal Diffusivity, mm2/s 23
12
Thermal Shock Resistance, points 14
22 to 23

Alloy Composition

Aluminum (Al), % 5.0 to 6.5
0
Arsenic (As), % 0.020 to 0.35
0
Copper (Cu), % 92.5 to 95
63.5 to 66.5
Iron (Fe), % 0 to 0.1
0 to 0.25
Lead (Pb), % 0 to 0.1
0 to 0.050
Manganese (Mn), % 0
0 to 0.5
Nickel (Ni), % 0
11 to 13
Zinc (Zn), % 0
19.2 to 25.5
Residuals, % 0
0 to 0.5