Mechanical Properties

Elastic (Young's, Tensile) Modulus, GPa 110
190
Elongation at Break, % 43
17 to 18
Poisson's Ratio 0.31
0.29
Shear Modulus, GPa 39
73
Shear Strength, MPa 240
360 to 410
Tensile Strength: Ultimate (UTS), MPa 350
590 to 670
Tensile Strength: Yield (Proof), MPa 120
350 to 360

Thermal Properties

Latent Heat of Fusion, J/g 180
260
Maximum Temperature: Mechanical, °C 140
410
Melting Completion (Liquidus), °C 930
1450
Melting Onset (Solidus), °C 910
1410
Specific Heat Capacity, J/kg-K 390
470
Thermal Conductivity, W/m-K 120
52
Thermal Expansion, µm/m-K 20
13

Electrical Properties

Electrical Conductivity: Equal Volume, % IACS 26
7.3
Electrical Conductivity: Equal Weight (Specific), % IACS 29
8.4

Otherwise Unclassified Properties

Base Metal Price, % relative 25
2.1
Density, g/cm3 8.2
7.8
Embodied Carbon, kg CO2/kg material 2.9
1.4
Embodied Energy, MJ/kg 48
19
Embodied Water, L/kg 320
49

Common Calculations

Resilience: Ultimate (Unit Rupture Work), MJ/m3 120
93 to 96
Resilience: Unit (Modulus of Resilience), kJ/m3 63
330 to 350
Stiffness to Weight: Axial, points 7.4
13
Stiffness to Weight: Bending, points 19
24
Strength to Weight: Axial, points 12
21 to 24
Strength to Weight: Bending, points 14
20 to 22
Thermal Diffusivity, mm2/s 37
14
Thermal Shock Resistance, points 12
17 to 20