MakeItFrom.com
Menu (ESC)

C95520 Bronze vs. ASTM A202 Steel

C95520 bronze belongs to the copper alloys classification, while ASTM A202 steel belongs to the iron alloys. There are 29 material properties with values for both materials. Properties with values for just one material (2, in this case) are not shown.

For each property being compared, the top bar is C95520 bronze and the bottom bar is ASTM A202 steel.

Metric UnitsUS Customary Units

Mechanical Properties

Brinell Hardness 280
180 to 200
Elastic (Young's, Tensile) Modulus, GPa 120
190
Elongation at Break, % 2.6
17 to 18
Poisson's Ratio 0.33
0.29
Shear Modulus, GPa 44
73
Tensile Strength: Ultimate (UTS), MPa 970
590 to 670
Tensile Strength: Yield (Proof), MPa 530
350 to 360

Thermal Properties

Latent Heat of Fusion, J/g 240
260
Maximum Temperature: Mechanical, °C 240
410
Melting Completion (Liquidus), °C 1070
1450
Melting Onset (Solidus), °C 1020
1410
Specific Heat Capacity, J/kg-K 450
470
Thermal Conductivity, W/m-K 40
52
Thermal Expansion, µm/m-K 18
13

Electrical Properties

Electrical Conductivity: Equal Volume, % IACS 11
7.3
Electrical Conductivity: Equal Weight (Specific), % IACS 12
8.4

Otherwise Unclassified Properties

Base Metal Price, % relative 29
2.1
Density, g/cm3 8.2
7.8
Embodied Carbon, kg CO2/kg material 3.6
1.4
Embodied Energy, MJ/kg 58
19
Embodied Water, L/kg 390
49

Common Calculations

Resilience: Ultimate (Unit Rupture Work), MJ/m3 21
93 to 96
Resilience: Unit (Modulus of Resilience), kJ/m3 1210
330 to 350
Stiffness to Weight: Axial, points 8.0
13
Stiffness to Weight: Bending, points 20
24
Strength to Weight: Axial, points 33
21 to 24
Strength to Weight: Bending, points 27
20 to 22
Thermal Diffusivity, mm2/s 11
14
Thermal Shock Resistance, points 33
17 to 20