MakeItFrom.com
Menu (ESC)

1060-H12 Aluminum

1060-H12 aluminum is 1060 aluminum in the H12 temper. To achieve this temper, the metal is strain hardened to a strength that is roughly a quarter of the way between annealed (O) and full-hard (H18). The graph bars on the material properties cards below compare 1060-H12 aluminum to: 1000-series alloys (top), all aluminum alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Brinell Hardness

23

Elastic (Young's, Tensile) Modulus

68 GPa 9.9 x 106 psi

Elongation at Break

12 %

Fatigue Strength

29 MPa 4.3 x 103 psi

Poisson's Ratio

0.33

Shear Modulus

26 GPa 3.7 x 106 psi

Shear Strength

55 MPa 8.0 x 103 psi

Tensile Strength: Ultimate (UTS)

85 MPa 12 x 103 psi

Tensile Strength: Yield (Proof)

61 MPa 8.9 x 103 psi

Thermal Properties

Latent Heat of Fusion

400 J/g

Maximum Temperature: Mechanical

170 °C 340 °F

Melting Completion (Liquidus)

660 °C 1210 °F

Melting Onset (Solidus)

650 °C 1190 °F

Specific Heat Capacity

900 J/kg-K 0.22 BTU/lb-°F

Thermal Conductivity

230 W/m-K 140 BTU/h-ft-°F

Thermal Expansion

24 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

62 % IACS

Electrical Conductivity: Equal Weight (Specific)

210 % IACS

Otherwise Unclassified Properties

Base Metal Price

9.5 % relative

Calomel Potential

-750 mV

Density

2.7 g/cm3 170 lb/ft3

Embodied Carbon

8.3 kg CO2/kg material

Embodied Energy

160 MJ/kg 67 x 103 BTU/lb

Embodied Water

1200 L/kg 140 gal/lb

Common Calculations

Resilience: Ultimate (Unit Rupture Work)

9.5 MJ/m3

Resilience: Unit (Modulus of Resilience)

27 kJ/m3

Stiffness to Weight: Axial

14 points

Stiffness to Weight: Bending

50 points

Strength to Weight: Axial

8.7 points

Strength to Weight: Bending

16 points

Thermal Diffusivity

96 mm2/s

Thermal Shock Resistance

3.8 points

Alloy Composition

Aluminum (Al)Al 99.6 to 100
Iron (Fe)Fe 0 to 0.35
Silicon (Si)Si 0 to 0.25
Zinc (Zn)Zn 0 to 0.050
Copper (Cu)Cu 0 to 0.050
Vanadium (V)V 0 to 0.050
Manganese (Mn)Mn 0 to 0.030
Titanium (Ti)Ti 0 to 0.030
Magnesium (Mg)Mg 0 to 0.030

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

ASTM B483: Standard Specification for Aluminum and Aluminum-Alloy Drawn Tube and Pipe for General Purpose Applications

ASTM B210: Standard Specification for Aluminum and Aluminum-Alloy Drawn Seamless Tubes

Handbook of Aluminum vol. 2: Alloy Production and Materials Manufacturing, George Totten and D. Scott MacKenzie (editors), 2003

ASTM B209: Standard Specification for Aluminum and Aluminum-Alloy Sheet and Plate

Aluminum Standards and Data, Aluminum Association Inc., 2013

ASM Specialty Handbook: Aluminum and Aluminum Alloys, J. R. Davis (editor), 1993

EN 573-3: Aluminium and aluminium alloys. Chemical composition and form of wrought products. Chemical composition and form of products