MakeItFrom.com
Menu (ESC)

1100A-H12 Aluminum

1100A-H12 aluminum is 1100A aluminum in the H12 temper. To achieve this temper, the metal is strain hardened to a strength that is roughly a quarter of the way between annealed (O) and full-hard (H18). The graph bars on the material properties cards below compare 1100A-H12 aluminum to: 1000-series alloys (top), all aluminum alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Elastic (Young's, Tensile) Modulus

69 GPa 10 x 106 psi

Elongation at Break

10 %

Fatigue Strength

65 MPa 9.4 x 103 psi

Poisson's Ratio

0.33

Shear Modulus

26 GPa 3.8 x 106 psi

Shear Strength

65 MPa 9.4 x 103 psi

Tensile Strength: Ultimate (UTS)

110 MPa 16 x 103 psi

Tensile Strength: Yield (Proof)

86 MPa 12 x 103 psi

Thermal Properties

Latent Heat of Fusion

400 J/g

Maximum Temperature: Mechanical

170 °C 340 °F

Melting Completion (Liquidus)

640 °C 1190 °F

Melting Onset (Solidus)

640 °C 1190 °F

Specific Heat Capacity

900 J/kg-K 0.22 BTU/lb-°F

Thermal Conductivity

230 W/m-K 130 BTU/h-ft-°F

Thermal Expansion

23 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

60 % IACS

Electrical Conductivity: Equal Weight (Specific)

200 % IACS

Otherwise Unclassified Properties

Base Metal Price

9.5 % relative

Density

2.7 g/cm3 170 lb/ft3

Embodied Carbon

8.2 kg CO2/kg material

Embodied Energy

150 MJ/kg 66 x 103 BTU/lb

Embodied Water

1190 L/kg 140 gal/lb

Common Calculations

Resilience: Ultimate (Unit Rupture Work)

10 MJ/m3

Resilience: Unit (Modulus of Resilience)

53 kJ/m3

Stiffness to Weight: Axial

14 points

Stiffness to Weight: Bending

50 points

Strength to Weight: Axial

11 points

Strength to Weight: Bending

19 points

Thermal Diffusivity

93 mm2/s

Thermal Shock Resistance

4.9 points

Alloy Composition

Aluminum (Al)Al 99 to 100
Silicon (Si)Si 0 to 1.0
Iron (Fe)Fe 0 to 1.0
Copper (Cu)Cu 0.050 to 0.2
Titanium (Ti)Ti 0 to 0.1
Zinc (Zn)Zn 0 to 0.1
Magnesium (Mg)Mg 0 to 0.1
Manganese (Mn)Mn 0 to 0.050
Residualsres. 0 to 0.15

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

Iron in Aluminium Alloys: Impurity and Alloying Element, N. A. Belov et al., 2002

ISO 6361-2: Wrought aluminium and aluminium alloys - Sheets, strips and plates - Part 2: Mechanical properties

CRC Materials Science and Engineering Handbook, 4th ed., James F. Shackelford et al. (editors), 2015