3/4-Hard (H03) C19500 Copper

H03 C19500 copper is C19500 copper in the H03 (3/4 hard) temper. It has the second lowest ductility compared to the other variants of C19500 copper. The graph bars on the material properties cards below compare H03 C19500 copper to: wrought coppers (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Elastic (Young's, Tensile) Modulus

120 GPa 17 x 106 psi

Elongation at Break

6.7 %

Poisson's Ratio

0.34

Rockwell B Hardness

82

Rockwell Superficial 30T Hardness

73

Shear Modulus

44 GPa 6.3 x 106 psi

Shear Strength

320 MPa 47 x 103 psi

Tensile Strength: Ultimate (UTS)

550 MPa 80 x 103 psi

Tensile Strength: Yield (Proof)

520 MPa 76 x 103 psi

Thermal Properties

Latent Heat of Fusion

210 J/g

Maximum Temperature: Mechanical

200 °C 390 °F

Melting Completion (Liquidus)

1090 °C 2000 °F

Melting Onset (Solidus)

1090 °C 1990 °F

Specific Heat Capacity

390 J/kg-K 0.092 BTU/lb-°F

Thermal Conductivity

200 W/m-K 120 BTU/h-ft-°F

Thermal Expansion

17 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

50 % IACS

Electrical Conductivity: Equal Weight (Specific)

51 % IACS

Otherwise Unclassified Properties

Base Metal Price

31 % relative

Density

8.9 g/cm3 560 lb/ft3

Embodied Carbon

2.7 kg CO2/kg material

Embodied Energy

42 MJ/kg 18 x 103 BTU/lb

Embodied Water

310 L/kg 37 gal/lb

Common Calculations

Resilience: Ultimate (Unit Rupture Work)

36 MJ/m3

Resilience: Unit (Modulus of Resilience)

1170 kJ/m3

Stiffness to Weight: Axial

7.3 points

Stiffness to Weight: Bending

18 points

Strength to Weight: Axial

17 points

Strength to Weight: Bending

17 points

Thermal Diffusivity

58 mm2/s

Thermal Shock Resistance

19 points

Alloy Composition

Copper (Cu)Cu 94.9 to 98.6
Iron (Fe)Fe 1.0 to 2.0
Cobalt (Co)Co 0.3 to 1.3
Tin (Sn)Sn 0.1 to 1.0
Phosphorus (P)P 0.010 to 0.35
Zinc (Zn)Zn 0 to 0.2
Aluminum (Al)Al 0 to 0.020
Lead (Pb)Pb 0 to 0.020
Residualsres. 0 to 0.2

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

ASTM B465: Standard Specification for Copper-Iron Alloy Plate, Sheet, Strip, and Rolled Bar