5252-H28 aluminum is 5252 aluminum in the H28 temper. This is the strongest temper normally produced through the action of strain hardening followed by partial annealing. It is closely related to H18. It has the lowest ductility compared to the other variants of 5252 aluminum.

The graph bars on the material properties cards below compare 5252-H28 aluminum to: 5000-series alloys (top), all aluminum alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Brinell Hardness

75

Elastic (Young's, Tensile) Modulus

68 GPa 9.8 x 106 psi

Elongation at Break

4.5 %

Fatigue Strength

100 MPa 15 x 103 psi

Poisson's Ratio

0.33

Shear Modulus

25 GPa 3.7 x 106 psi

Shear Strength

160 MPa 23 x 103 psi

Tensile Strength: Ultimate (UTS)

290 MPa 42 x 103 psi

Tensile Strength: Yield (Proof)

240 MPa 35 x 103 psi

Thermal Properties

Latent Heat of Fusion

400 J/g

Maximum Temperature: Mechanical

180 °C 360 °F

Melting Completion (Liquidus)

650 °C 1200 °F

Melting Onset (Solidus)

610 °C 1120 °F

Specific Heat Capacity

910 J/kg-K 0.22 BTU/lb-°F

Thermal Conductivity

140 W/m-K 80 BTU/h-ft-°F

Thermal Expansion

24 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

34 % IACS

Electrical Conductivity: Equal Weight (Specific)

120 % IACS

Otherwise Unclassified Properties

Base Metal Price

9.5 % relative

Density

2.7 g/cm3 170 lb/ft3

Embodied Carbon

8.7 kg CO2/kg material

Embodied Energy

160 MJ/kg 67 x 103 BTU/lb

Embodied Water

1190 L/kg 140 gal/lb

Common Calculations

Resilience: Ultimate (Unit Rupture Work)

12 MJ/m3

Resilience: Unit (Modulus of Resilience)

430 kJ/m3

Stiffness to Weight: Axial

14 points

Stiffness to Weight: Bending

51 points

Strength to Weight: Axial

30 points

Strength to Weight: Bending

36 points

Thermal Diffusivity

57 mm2/s

Thermal Shock Resistance

13 points

Alloy Composition

Aluminum (Al)Al 96.6 to 97.8
Magnesium (Mg)Mg 2.2 to 2.8
Manganese (Mn)Mn 0 to 0.1
Iron (Fe)Fe 0 to 0.1
Copper (Cu)Cu 0 to 0.1
Silicon (Si)Si 0 to 0.080
Zinc (Zn)Zn 0 to 0.050
Vanadium (V)V 0 to 0.050
Residualsres. 0 to 0.1

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

ASTM B209: Standard Specification for Aluminum and Aluminum-Alloy Sheet and Plate

Aluminum Standards and Data, Aluminum Association Inc., 2013

ASM Specialty Handbook: Aluminum and Aluminum Alloys, J. R. Davis (editor), 1993

EN 573-3: Aluminium and aluminium alloys. Chemical composition and form of wrought products. Chemical composition and form of products