5383-H116 Aluminum

5383-H116 aluminum is 5383 aluminum in the H116 temper. To achieve this temper, the metal is treated in whatever manner is required to develop a particular degree of intergranular and exfoliation corrosion.

The graph bars on the material properties cards below compare 5383-H116 aluminum to: 5000-series alloys (top), all aluminum alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Brinell Hardness

90

Elastic (Young's, Tensile) Modulus

68 GPa 9.9 x 106 psi

Elongation at Break

12 %

Fatigue Strength

170 MPa 25 x 103 psi

Poisson's Ratio

0.33

Shear Modulus

26 GPa 3.7 x 106 psi

Shear Strength

210 MPa 30 x 103 psi

Tensile Strength: Ultimate (UTS)

350 MPa 51 x 103 psi

Tensile Strength: Yield (Proof)

240 MPa 35 x 103 psi

Thermal Properties

Latent Heat of Fusion

390 J/g

Maximum Temperature: Corrosion

65 °C 150 °F

Maximum Temperature: Mechanical

200 °C 400 °F

Melting Completion (Liquidus)

650 °C 1200 °F

Melting Onset (Solidus)

540 °C 1010 °F

Specific Heat Capacity

900 J/kg-K 0.22 BTU/lb-°F

Thermal Conductivity

130 W/m-K 72 BTU/h-ft-°F

Thermal Expansion

24 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

29 % IACS

Electrical Conductivity: Equal Weight (Specific)

97 % IACS

Otherwise Unclassified Properties

Base Metal Price

9.5 % relative

Density

2.7 g/cm3 170 lb/ft3

Embodied Carbon

9.0 kg CO2/kg material

Embodied Energy

160 MJ/kg 67 x 103 BTU/lb

Embodied Water

1170 L/kg 140 gal/lb

Common Calculations

Resilience: Ultimate (Unit Rupture Work)

38 MJ/m3

Resilience: Unit (Modulus of Resilience)

440 kJ/m3

Stiffness to Weight: Axial

14 points

Stiffness to Weight: Bending

50 points

Strength to Weight: Axial

36 points

Strength to Weight: Bending

41 points

Thermal Diffusivity

51 mm2/s

Thermal Shock Resistance

15 points

Alloy Composition

Aluminum (Al)Al 92 to 95.3
Magnesium (Mg)Mg 4.0 to 5.2
Manganese (Mn)Mn 0.7 to 1.0
Zinc (Zn)Zn 0 to 0.4
Silicon (Si)Si 0 to 0.25
Chromium (Cr)Cr 0 to 0.25
Iron (Fe)Fe 0 to 0.25
Zirconium (Zr)Zr 0 to 0.2
Copper (Cu)Cu 0 to 0.2
Titanium (Ti)Ti 0 to 0.15
Residualsres. 0 to 0.15

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

ASTM B928: Standard Specification for High Magnesium Aluminum-Alloy Sheet and Plate for Marine Service

EN 485-2: Aluminium and aluminium alloys. Sheet, strip and plate. Mechanical properties

ISO 6361-2: Wrought aluminium and aluminium alloys - Sheets, strips and plates - Part 2: Mechanical properties

EN 573-3: Aluminium and aluminium alloys. Chemical composition and form of wrought products. Chemical composition and form of products

Properties and Selection: Nonferrous Alloys and Special-Purpose Materials, ASM Handbook vol. 2, ASM International, 1993

CRC Materials Science and Engineering Handbook, 4th ed., James F. Shackelford et al. (editors), 2015