6101-T65 Aluminum

6101-T65 aluminum is 6101 aluminum in the T65 temper. To achieve this temper, the metal is solution heat-treated and artificially underaged. The degree of underaging is different from T61 and T64. The graph bars on the material properties cards below compare 6101-T65 aluminum to: 6000-series alloys (top), all aluminum alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Elastic (Young's, Tensile) Modulus

68 GPa 9.9 x 106 psi

Poisson's Ratio

0.33

Shear Modulus

26 GPa 3.7 x 106 psi

Thermal Properties

Latent Heat of Fusion

400 J/g

Maximum Temperature: Mechanical

160 °C 320 °F

Melting Completion (Liquidus)

650 °C 1210 °F

Melting Onset (Solidus)

620 °C 1150 °F

Specific Heat Capacity

900 J/kg-K 0.22 BTU/lb-°F

Thermal Conductivity

220 W/m-K 130 BTU/h-ft-°F

Thermal Expansion

23 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

58 % IACS

Electrical Conductivity: Equal Weight (Specific)

190 % IACS

Otherwise Unclassified Properties

Base Metal Price

9.5 % relative

Density

2.7 g/cm3 170 lb/ft3

Embodied Carbon

8.3 kg CO2/kg material

Embodied Energy

150 MJ/kg 66 x 103 BTU/lb

Embodied Water

1190 L/kg 140 gal/lb

Common Calculations

Stiffness to Weight: Axial

14 points

Stiffness to Weight: Bending

50 points

Thermal Diffusivity

89 mm2/s

Alloy Composition

Aluminum (Al)Al 97.6 to 99.4
Magnesium (Mg)Mg 0.35 to 0.8
Silicon (Si)Si 0.3 to 0.7
Iron (Fe)Fe 0 to 0.5
Zinc (Zn)Zn 0 to 0.1
Copper (Cu)Cu 0 to 0.1
Boron (B)B 0 to 0.060
Manganese (Mn)Mn 0 to 0.030
Chromium (Cr)Cr 0 to 0.030
Residualsres. 0 to 0.1

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

Aluminum Standards and Data, Aluminum Association Inc., 2013

ASM Specialty Handbook: Aluminum and Aluminum Alloys, J. R. Davis (editor), 1993

EN 573-3: Aluminium and aluminium alloys. Chemical composition and form of wrought products. Chemical composition and form of products