As Forged and Quenched (M11) C67600 Bronze

M11 C67600 bronze is C67600 bronze in the M11 (as forged and quenched) condition. The graph bars on the material properties cards below compare M11 C67600 bronze to: wrought bronzes (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Elastic (Young's, Tensile) Modulus

100 GPa 15 x 106 psi

Elongation at Break

33 %

Poisson's Ratio

0.31

Rockwell B Hardness

69

Shear Modulus

40 GPa 5.8 x 106 psi

Shear Strength

330 MPa 48 x 103 psi

Tensile Strength: Ultimate (UTS)

500 MPa 72 x 103 psi

Tensile Strength: Yield (Proof)

240 MPa 34 x 103 psi

Thermal Properties

Latent Heat of Fusion

170 J/g

Maximum Temperature: Mechanical

120 °C 240 °F

Melting Completion (Liquidus)

890 °C 1630 °F

Melting Onset (Solidus)

870 °C 1590 °F

Specific Heat Capacity

380 J/kg-K 0.092 BTU/lb-°F

Thermal Conductivity

110 W/m-K 61 BTU/h-ft-°F

Thermal Expansion

21 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

24 % IACS

Electrical Conductivity: Equal Weight (Specific)

27 % IACS

Otherwise Unclassified Properties

Base Metal Price

23 % relative

Density

8.0 g/cm3 500 lb/ft3

Embodied Carbon

2.8 kg CO2/kg material

Embodied Energy

47 MJ/kg 20 x 103 BTU/lb

Embodied Water

330 L/kg 39 gal/lb

Common Calculations

Resilience: Ultimate (Unit Rupture Work)

130 MJ/m3

Resilience: Unit (Modulus of Resilience)

270 kJ/m3

Stiffness to Weight: Axial

7.2 points

Stiffness to Weight: Bending

20 points

Strength to Weight: Axial

17 points

Strength to Weight: Bending

17 points

Thermal Diffusivity

35 mm2/s

Thermal Shock Resistance

16 points

Alloy Composition

Copper (Cu)Cu 57 to 60
Zinc (Zn)Zn 35.2 to 41.6
Tin (Sn)Sn 0.5 to 1.5
Iron (Fe)Fe 0.4 to 1.3
Lead (Pb)Pb 0.5 to 1.0
Manganese (Mn)Mn 0.050 to 0.5
Residualsres. 0 to 0.5

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

ASTM B283: Standard Specification for Copper and Copper-Alloy Die Forgings (Hot-Pressed)

ASTM B124: Standard Specification for Copper and Copper Alloy Forging Rod, Bar, and Shapes

ASM Specialty Handbook: Copper and Copper Alloys, J. R. Davis (editor), 2001