MakeItFrom.com
Menu (ESC)

Baria-Alkali-Silica Glass (IEC 60672 Type G-600)

Baria-alkali-silica glass is a glass-type material. It has a fairly high density among the glass and glass-ceramics in the database. The graph bars on the material properties cards below compare baria-alkali-silica glass to other glass and glass-ceramics (top) and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Thermal Properties

Glass Transition Temperature

470 °C 870 °F

Thermal Expansion

9.5 µm/m-K

Electrical Properties

Dielectric Constant (Relative Permittivity) At 1 Hz

7.0

Electrical Dissipation At 1 Hz

0.0034

Electrical Dissipation At 1 MHz

0.0022

Electrical Resistivity Order of Magnitude

12 10x Ω-m

Other Material Properties

Density

3.0 g/cm3 190 lb/ft3

Elastic (Young's, Tensile) Modulus

80 GPa 12 x 106 psi

Flexural Strength

34 MPa 4.9 x 103 psi

Common Calculations

Stiffness to Weight: Axial

15 points

Stiffness to Weight: Bending

48 points

Followup Questions

Further Reading

Glass: Mechanics and Technology, Eric Le Bourhis, 2007

Handbook of Optical Materials, Marvin J. Weber, 2003

IEC 60672-3: Ceramic and glass-insulating materials - Part 3: Specifications for individual materials