EN AC-43500-F is EN AC-43500 aluminum in the as-fabricated (no temper or treatment) condition. The graph bars on the material properties cards below compare EN AC-43500-F to: Euronorm (EN) cast aluminums (top), all aluminum alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Brinell Hardness

74

Elastic (Young's, Tensile) Modulus

72 GPa 10 x 106 psi

Elongation at Break

5.6 %

Fatigue Strength

100 MPa 15 x 103 psi

Poisson's Ratio

0.33

Shear Modulus

27 GPa 3.9 x 106 psi

Tensile Strength: Ultimate (UTS)

280 MPa 41 x 103 psi

Tensile Strength: Yield (Proof)

140 MPa 20 x 103 psi

Thermal Properties

Latent Heat of Fusion

550 J/g

Maximum Temperature: Mechanical

170 °C 340 °F

Melting Completion (Liquidus)

600 °C 1100 °F

Melting Onset (Solidus)

590 °C 1090 °F

Specific Heat Capacity

900 J/kg-K 0.22 BTU/lb-°F

Thermal Conductivity

140 W/m-K 80 BTU/h-ft-°F

Thermal Expansion

22 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

38 % IACS

Electrical Conductivity: Equal Weight (Specific)

130 % IACS

Otherwise Unclassified Properties

Base Metal Price

9.5 % relative

Density

2.6 g/cm3 160 lb/ft3

Embodied Carbon

7.8 kg CO2/kg material

Embodied Energy

150 MJ/kg 63 x 103 BTU/lb

Embodied Water

1070 L/kg 130 gal/lb

Common Calculations

Resilience: Ultimate (Unit Rupture Work)

13 MJ/m3

Resilience: Unit (Modulus of Resilience)

130 kJ/m3

Stiffness to Weight: Axial

16 points

Stiffness to Weight: Bending

54 points

Strength to Weight: Axial

30 points

Strength to Weight: Bending

37 points

Thermal Diffusivity

60 mm2/s

Thermal Shock Resistance

13 points

Alloy Composition

Aluminum (Al)Al 86.4 to 90.5
Silicon (Si)Si 9.0 to 11.5
Manganese (Mn)Mn 0.4 to 0.8
Magnesium (Mg)Mg 0.1 to 0.6
Iron (Fe)Fe 0 to 0.25
Titanium (Ti)Ti 0 to 0.2
Zinc (Zn)Zn 0 to 0.070
Copper (Cu)Cu 0 to 0.050
Residualsres. 0 to 0.15

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

EN 1706: Aluminium and aluminium alloys. Castings. Chemical composition and mechanical properties

Aluminum: Properties and Physical Metallurgy, John E. Hatch (editor), 1984