MakeItFrom.com
Menu (ESC)

Extra-Hard (H06) C19200 Copper

H06 C19200 copper is C19200 copper in the H06 (extra hard) temper. The graph bars on the material properties cards below compare H06 C19200 copper to: wrought coppers (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Elastic (Young's, Tensile) Modulus

120 GPa 17 x 106 psi

Elongation at Break

3.0 %

Poisson's Ratio

0.34

Rockwell B Hardness

74

Rockwell Superficial 30T Hardness

71

Shear Modulus

44 GPa 6.3 x 106 psi

Shear Strength

280 MPa 40 x 103 psi

Tensile Strength: Ultimate (UTS)

480 MPa 70 x 103 psi

Tensile Strength: Yield (Proof)

460 MPa 66 x 103 psi

Thermal Properties

Latent Heat of Fusion

210 J/g

Maximum Temperature: Mechanical

200 °C 390 °F

Melting Completion (Liquidus)

1080 °C 1980 °F

Melting Onset (Solidus)

1080 °C 1970 °F

Specific Heat Capacity

390 J/kg-K 0.092 BTU/lb-°F

Thermal Conductivity

240 W/m-K 140 BTU/h-ft-°F

Thermal Expansion

17 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

68 % IACS

Electrical Conductivity: Equal Weight (Specific)

69 % IACS

Otherwise Unclassified Properties

Base Metal Price

30 % relative

Density

8.9 g/cm3 560 lb/ft3

Embodied Carbon

2.6 kg CO2/kg material

Embodied Energy

41 MJ/kg 18 x 103 BTU/lb

Embodied Water

310 L/kg 37 gal/lb

Common Calculations

Resilience: Ultimate (Unit Rupture Work)

14 MJ/m3

Resilience: Unit (Modulus of Resilience)

890 kJ/m3

Stiffness to Weight: Axial

7.2 points

Stiffness to Weight: Bending

18 points

Strength to Weight: Axial

15 points

Strength to Weight: Bending

15 points

Thermal Diffusivity

69 mm2/s

Thermal Shock Resistance

17 points

Alloy Composition

Copper (Cu)Cu 98.5 to 99.19
Iron (Fe)Fe 0.8 to 1.2
Zinc (Zn)Zn 0 to 0.2
Phosphorus (P)P 0.010 to 0.040
Lead (Pb)Pb 0 to 0.030
Residualsres. 0 to 0.2

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

ASTM B465: Standard Specification for Copper-Iron Alloy Plate, Sheet, Strip, and Rolled Bar