Extra-Spring (H10) C10400 Copper

H10 C10400 copper is C10400 copper in the H10 (extra spring) temper. It has the highest strength compared to the other variants of C10400 copper. The graph bars on the material properties cards below compare H10 C10400 copper to: wrought coppers (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Elastic (Young's, Tensile) Modulus

120 GPa 17 x 106 psi

Elongation at Break

3.3 %

Poisson's Ratio

0.34

Rockwell F Hardness

100

Rockwell Superficial 30T Hardness

70

Shear Modulus

43 GPa 6.3 x 106 psi

Shear Strength

240 MPa 34 x 103 psi

Tensile Strength: Ultimate (UTS)

410 MPa 60 x 103 psi

Tensile Strength: Yield (Proof)

400 MPa 58 x 103 psi

Thermal Properties

Latent Heat of Fusion

210 J/g

Maximum Temperature: Mechanical

200 °C 390 °F

Melting Completion (Liquidus)

1080 °C 1980 °F

Melting Onset (Solidus)

1080 °C 1980 °F

Specific Heat Capacity

390 J/kg-K 0.092 BTU/lb-°F

Thermal Conductivity

390 W/m-K 220 BTU/h-ft-°F

Thermal Expansion

17 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

100 % IACS

Electrical Conductivity: Equal Weight (Specific)

100 % IACS

Otherwise Unclassified Properties

Base Metal Price

32 % relative

Density

9.0 g/cm3 560 lb/ft3

Embodied Carbon

2.6 kg CO2/kg material

Embodied Energy

42 MJ/kg 18 x 103 BTU/lb

Embodied Water

340 L/kg 40 gal/lb

Common Calculations

Resilience: Ultimate (Unit Rupture Work)

13 MJ/m3

Resilience: Unit (Modulus of Resilience)

690 kJ/m3

Stiffness to Weight: Axial

7.2 points

Stiffness to Weight: Bending

18 points

Strength to Weight: Axial

13 points

Strength to Weight: Bending

14 points

Thermal Diffusivity

110 mm2/s

Thermal Shock Resistance

15 points

Alloy Composition

Copper (Cu)Cu 99.9 to 99.973
Silver (Ag)Ag 0.027 to 0.050
Oxygen (O)O 0 to 0.0010
Residualsres. 0 to 0.050

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

ASTM B152: Standard Specification for Copper Sheet, Strip, Plate, and Rolled Bar

Copper: Its Trade, Manufacture, Use, and Environmental Status, Gunter Joseph, 2001

ASM Specialty Handbook: Copper and Copper Alloys, J. R. Davis (editor), 2001