Extra-Spring (H10) C51100 Bronze

H10 C51100 bronze is C51100 bronze in the H10 (extra spring) temper. It has the highest strength and lowest ductility compared to the other variants of C51100 bronze. The graph bars on the material properties cards below compare H10 C51100 bronze to: wrought bronzes (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Elastic (Young's, Tensile) Modulus

110 GPa 16 x 106 psi

Elongation at Break

2.5 %

Poisson's Ratio

0.34

Rockwell B Hardness

93

Rockwell Superficial 30T Hardness

79

Shear Modulus

42 GPa 6.1 x 106 psi

Shear Strength

410 MPa 59 x 103 psi

Tensile Strength: Ultimate (UTS)

720 MPa 100 x 103 psi

Tensile Strength: Yield (Proof)

700 MPa 100 x 103 psi

Thermal Properties

Latent Heat of Fusion

200 J/g

Maximum Temperature: Mechanical

190 °C 370 °F

Melting Completion (Liquidus)

1060 °C 1950 °F

Melting Onset (Solidus)

970 °C 1790 °F

Specific Heat Capacity

380 J/kg-K 0.090 BTU/lb-°F

Thermal Conductivity

84 W/m-K 49 BTU/h-ft-°F

Thermal Expansion

18 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

20 % IACS

Electrical Conductivity: Equal Weight (Specific)

20 % IACS

Otherwise Unclassified Properties

Base Metal Price

32 % relative

Density

8.9 g/cm3 550 lb/ft3

Embodied Carbon

3.0 kg CO2/kg material

Embodied Energy

48 MJ/kg 21 x 103 BTU/lb

Embodied Water

340 L/kg 41 gal/lb

Common Calculations

Resilience: Ultimate (Unit Rupture Work)

18 MJ/m3

Resilience: Unit (Modulus of Resilience)

2170 kJ/m3

Stiffness to Weight: Axial

7.1 points

Stiffness to Weight: Bending

18 points

Strength to Weight: Axial

22 points

Strength to Weight: Bending

20 points

Thermal Diffusivity

25 mm2/s

Thermal Shock Resistance

26 points

Alloy Composition

Copper (Cu)Cu 93.8 to 96.5
Tin (Sn)Sn 3.5 to 4.9
Phosphorus (P)P 0.030 to 0.35
Zinc (Zn)Zn 0 to 0.3
Iron (Fe)Fe 0 to 0.1
Lead (Pb)Pb 0 to 0.050
Residualsres. 0 to 0.5

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

ASTM B103: Standard Specification for Phosphor Bronze Plate, Sheet, Strip, and Rolled Bar

ASM Specialty Handbook: Copper and Copper Alloys, J. R. Davis (editor), 2001