H04 C11000 copper is C11000 copper in the H04 (full hard) temper. The graph bars on the material properties cards below compare H04 C11000 copper to: wrought coppers (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Elastic (Young's, Tensile) Modulus

120 GPa 17 x 106 psi

Elongation at Break

20 %

Poisson's Ratio

0.34

Rockwell B Hardness

45

Rockwell F Hardness

87

Rockwell Superficial 30T Hardness

58

Shear Modulus

43 GPa 6.3 x 106 psi

Shear Strength

180 MPa 26 x 103 psi

Tensile Strength: Ultimate (UTS)

320 MPa 46 x 103 psi

Tensile Strength: Yield (Proof)

280 MPa 40 x 103 psi

Thermal Properties

Latent Heat of Fusion

210 J/g

Maximum Temperature: Mechanical

200 °C 390 °F

Melting Completion (Liquidus)

1080 °C 1980 °F

Melting Onset (Solidus)

1070 °C 1950 °F

Specific Heat Capacity

390 J/kg-K 0.092 BTU/lb-°F

Thermal Conductivity

390 W/m-K 230 BTU/h-ft-°F

Thermal Expansion

17 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

100 % IACS

Electrical Conductivity: Equal Weight (Specific)

100 % IACS

Otherwise Unclassified Properties

Base Metal Price

31 % relative

Density

9.0 g/cm3 560 lb/ft3

Embodied Carbon

2.6 kg CO2/kg material

Embodied Energy

41 MJ/kg 18 x 103 BTU/lb

Embodied Water

310 L/kg 37 gal/lb

Common Calculations

Resilience: Ultimate (Unit Rupture Work)

61 MJ/m3

Resilience: Unit (Modulus of Resilience)

330 kJ/m3

Stiffness to Weight: Axial

7.2 points

Stiffness to Weight: Bending

18 points

Strength to Weight: Axial

9.9 points

Strength to Weight: Bending

12 points

Thermal Diffusivity

110 mm2/s

Thermal Shock Resistance

12 points

Alloy Composition

Copper (Cu)Cu 99.9 to 100
Residualsres. 0 to 0.1

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

ASTM B124: Standard Specification for Copper and Copper Alloy Forging Rod, Bar, and Shapes

ASTM B283: Standard Specification for Copper and Copper-Alloy Die Forgings (Hot-Pressed)

ASTM B152: Standard Specification for Copper Sheet, Strip, Plate, and Rolled Bar

Copper Alloys: Preparation, Properties and Applications, Michael Naboka and Jennifer Giordano (editors), 2013

Copper: Its Trade, Manufacture, Use, and Environmental Status, Gunter Joseph, 2001

Properties and Selection: Nonferrous Alloys and Special-Purpose Materials, ASM Handbook vol. 2, ASM International, 1993