Full-Hard (H04) C26200 Brass

H04 C26200 brass is C26200 brass in the H04 (full hard) temper. The graph bars on the material properties cards below compare H04 C26200 brass to: wrought brasses (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Elastic (Young's, Tensile) Modulus

110 GPa 15 x 106 psi

Elongation at Break

8.0 %

Fatigue Strength

140 MPa 21 x 103 psi

Poisson's Ratio

0.31

Rockwell B Hardness

82

Rockwell Superficial 30T Hardness

73

Shear Modulus

41 GPa 5.9 x 106 psi

Shear Strength

300 MPa 44 x 103 psi

Tensile Strength: Ultimate (UTS)

530 MPa 77 x 103 psi

Tensile Strength: Yield (Proof)

480 MPa 69 x 103 psi

Thermal Properties

Latent Heat of Fusion

180 J/g

Maximum Temperature: Mechanical

140 °C 280 °F

Melting Completion (Liquidus)

950 °C 1750 °F

Melting Onset (Solidus)

920 °C 1680 °F

Specific Heat Capacity

390 J/kg-K 0.092 BTU/lb-°F

Thermal Conductivity

120 W/m-K 70 BTU/h-ft-°F

Thermal Expansion

20 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

28 % IACS

Electrical Conductivity: Equal Weight (Specific)

31 % IACS

Otherwise Unclassified Properties

Base Metal Price

25 % relative

Density

8.2 g/cm3 510 lb/ft3

Embodied Carbon

2.7 kg CO2/kg material

Embodied Energy

45 MJ/kg 19 x 103 BTU/lb

Embodied Water

320 L/kg 38 gal/lb

Common Calculations

Resilience: Ultimate (Unit Rupture Work)

41 MJ/m3

Resilience: Unit (Modulus of Resilience)

1060 kJ/m3

Stiffness to Weight: Axial

7.2 points

Stiffness to Weight: Bending

19 points

Strength to Weight: Axial

18 points

Strength to Weight: Bending

18 points

Thermal Diffusivity

38 mm2/s

Thermal Shock Resistance

18 points

Alloy Composition

Copper (Cu)Cu 67 to 70
Zinc (Zn)Zn 29.6 to 33
Lead (Pb)Pb 0 to 0.070
Iron (Fe)Fe 0 to 0.050
Residualsres. 0 to 0.3

All values are % weight. Ranges represent what is permitted under applicable standards.