Half-Hard (H02) C18700 Copper

H02 C18700 copper is C18700 copper in the H02 (half hard) temper. The graph bars on the material properties cards below compare H02 C18700 copper to: wrought coppers (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Elastic (Young's, Tensile) Modulus

110 GPa 17 x 106 psi

Elongation at Break

9.0 %

Poisson's Ratio

0.34

Shear Modulus

43 GPa 6.2 x 106 psi

Shear Strength

170 MPa 25 x 103 psi

Tensile Strength: Ultimate (UTS)

290 MPa 42 x 103 psi

Tensile Strength: Yield (Proof)

230 MPa 34 x 103 psi

Thermal Properties

Latent Heat of Fusion

210 J/g

Maximum Temperature: Mechanical

200 °C 390 °F

Melting Completion (Liquidus)

1080 °C 1980 °F

Melting Onset (Solidus)

950 °C 1750 °F

Specific Heat Capacity

380 J/kg-K 0.091 BTU/lb-°F

Thermal Conductivity

380 W/m-K 220 BTU/h-ft-°F

Thermal Expansion

17 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

98 % IACS

Electrical Conductivity: Equal Weight (Specific)

99 % IACS

Otherwise Unclassified Properties

Base Metal Price

30 % relative

Density

9.0 g/cm3 560 lb/ft3

Embodied Carbon

2.6 kg CO2/kg material

Embodied Energy

41 MJ/kg 18 x 103 BTU/lb

Embodied Water

310 L/kg 37 gal/lb

Common Calculations

Resilience: Ultimate (Unit Rupture Work)

24 MJ/m3

Resilience: Unit (Modulus of Resilience)

240 kJ/m3

Stiffness to Weight: Axial

7.1 points

Stiffness to Weight: Bending

18 points

Strength to Weight: Axial

9.0 points

Strength to Weight: Bending

11 points

Thermal Diffusivity

110 mm2/s

Thermal Shock Resistance

10 points

Alloy Composition

Copper (Cu)Cu 98 to 99.2
Lead (Pb)Pb 0.8 to 1.5
Residualsres. 0 to 0.5

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

ASTM B301: Standard Specification for Free-Cutting Copper Rod, Bar, Wire, and Shapes

Copper Alloys: Preparation, Properties and Applications, Michael Naboka and Jennifer Giordano (editors), 2013

ASM Specialty Handbook: Copper and Copper Alloys, J. R. Davis (editor), 2001