Quenched and Tempered (+QT2) 1.7710 Cast Steel

EN 1.7710 +QT2 steel is EN 1.7710 steel in the quenched and tempered condition. The graph bars on the material properties cards below compare EN 1.7710 +QT2 steel to: cast alloy steels (top), all iron alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Brinell Hardness

320

Elastic (Young's, Tensile) Modulus

190 GPa 27 x 106 psi

Elongation at Break

6.8 %

Fatigue Strength

620 MPa 90 x 103 psi

Impact Strength: V-Notched Charpy

30 J 22 ft-lb

Poisson's Ratio

0.29

Shear Modulus

73 GPa 11 x 106 psi

Tensile Strength: Ultimate (UTS)

1070 MPa 150 x 103 psi

Tensile Strength: Yield (Proof)

1060 MPa 150 x 103 psi

Thermal Properties

Latent Heat of Fusion

260 J/g

Maximum Temperature: Mechanical

440 °C 830 °F

Melting Completion (Liquidus)

1470 °C 2670 °F

Melting Onset (Solidus)

1430 °C 2600 °F

Specific Heat Capacity

470 J/kg-K 0.11 BTU/lb-°F

Thermal Conductivity

41 W/m-K 24 BTU/h-ft-°F

Thermal Expansion

13 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

7.5 % IACS

Electrical Conductivity: Equal Weight (Specific)

8.6 % IACS

Otherwise Unclassified Properties

Base Metal Price

3.5 % relative

Density

7.8 g/cm3 490 lb/ft3

Embodied Carbon

2.2 kg CO2/kg material

Embodied Energy

30 MJ/kg 13 x 103 BTU/lb

Embodied Water

57 L/kg 6.8 gal/lb

Common Calculations

PREN (Pitting Resistance)

4.5

Resilience: Ultimate (Unit Rupture Work)

73 MJ/m3

Resilience: Unit (Modulus of Resilience)

2970 kJ/m3

Stiffness to Weight: Axial

13 points

Stiffness to Weight: Bending

24 points

Strength to Weight: Axial

38 points

Strength to Weight: Bending

30 points

Thermal Diffusivity

11 mm2/s

Thermal Shock Resistance

31 points

Alloy Composition

Iron (Fe)Fe 95.1 to 97
Chromium (Cr)Cr 1.3 to 1.8
Molybdenum (Mo)Mo 0.8 to 1.0
Manganese (Mn)Mn 0.6 to 1.0
Silicon (Si)Si 0 to 0.6
Vanadium (V)V 0.15 to 0.25
Carbon (C)C 0.12 to 0.18
Sulfur (S)S 0 to 0.030
Phosphorus (P)P 0 to 0.025

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

EN 10293: Steel castings - Steel castings for general engineering uses

Properties and Selection: Irons, Steels and High Performance Alloys, ASM Handbook vol. 1, ASM International, 1993

Manufacture and Uses of Alloy Steels, Henry D. Hibbard, 2005

Ferrous Materials: Steel and Cast Iron, Hans Berns and Werner Theisen, 2008

Steels: Processing, Structure, and Performance, 2nd ed., George Krauss, 2015