30% Glass Fiber (30 GF) PPO

30 GF PPO is a grade of PPO. The graph bars on the material properties cards below compare 30 GF PPO to: polyphenylene plastics (top), all thermoplastics (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Flexural Modulus

7.6 GPa 1.1 x 106 psi

Flexural Strength

140 MPa 20 x 103 psi

Impact Strength: Notched Izod

120 J/m 2.3 ft-lb/in

Tensile Strength: Ultimate (UTS)

120 MPa 18 x 103 psi

Thermal Properties

Heat Deflection Temperature At 1.82 MPa (264 psi)

140 °C 280 °F

Maximum Temperature: Mechanical

110 °C 220 °F

Specific Heat Capacity

1070 J/kg-K 0.26 BTU/lb-°F

Thermal Expansion

25 µm/m-K

Electrical Properties

Dielectric Constant (Relative Permittivity) At 1 Hz

3.2

Dielectric Strength (Breakdown Potential)

21 kV/mm 0.82 V/mil

Electrical Dissipation At 1 Hz

0.0020

Electrical Resistivity Order of Magnitude

15 10x Ω-m

Otherwise Unclassified Properties

Density

1.4 g/cm3 85 lb/ft3

Limiting Oxygen Index (LOI)

32 %

Water Absorption After 24 Hours

0.060 %

Common Calculations

Strength to Weight: Axial

25 points

Strength to Weight: Bending

40 points

Followup Questions

Further Reading

Reinforced Plastics Durability, Geoffrey Pritchard (editor), 1999

SPI Plastics Engineering Handbook of the Society of the Plastics Industry, Inc., 5th ed., Michael L. Berins (editor), 2000

Modern Plastics Handbook, Charles A. Harper (editor), 1999

Plastics Materials, 7th ed., J. A. Brydson, 1999

CRC Materials Science and Engineering Handbook, 4th ed., James F. Shackelford et al. (editors), 2015