710.0-T1 aluminum is 710.0 aluminum in the T1 temper. To achieve this temper, the metal is naturally aged until it meets standard mechanical property requirements. The graph bars on the material properties cards below compare 710.0-T1 aluminum to: ANSI/AA cast aluminums (top), all aluminum alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Brinell Hardness

75

Elastic (Young's, Tensile) Modulus

70 GPa 10 x 106 psi

Elongation at Break

2.2 %

Fatigue Strength

110 MPa 15 x 103 psi

Poisson's Ratio

0.32

Shear Modulus

26 GPa 3.8 x 106 psi

Tensile Strength: Ultimate (UTS)

250 MPa 36 x 103 psi

Tensile Strength: Yield (Proof)

160 MPa 23 x 103 psi

Thermal Properties

Latent Heat of Fusion

380 J/g

Maximum Temperature: Mechanical

170 °C 340 °F

Melting Completion (Liquidus)

650 °C 1200 °F

Melting Onset (Solidus)

610 °C 1120 °F

Solidification (Pattern Maker's) Shrinkage

1.6 %

Specific Heat Capacity

870 J/kg-K 0.21 BTU/lb-°F

Thermal Conductivity

140 W/m-K 79 BTU/h-ft-°F

Thermal Expansion

24 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

35 % IACS

Electrical Conductivity: Equal Weight (Specific)

110 % IACS

Otherwise Unclassified Properties

Base Metal Price

9.5 % relative

Density

3.0 g/cm3 190 lb/ft3

Embodied Carbon

8.0 kg CO2/kg material

Embodied Energy

150 MJ/kg 64 x 103 BTU/lb

Embodied Water

1130 L/kg 140 gal/lb

Common Calculations

Resilience: Ultimate (Unit Rupture Work)

4.9 MJ/m3

Resilience: Unit (Modulus of Resilience)

180 kJ/m3

Stiffness to Weight: Axial

13 points

Stiffness to Weight: Bending

46 points

Strength to Weight: Axial

23 points

Strength to Weight: Bending

29 points

Thermal Diffusivity

53 mm2/s

Thermal Shock Resistance

11 points

Alloy Composition

Aluminum (Al)Al 90.5 to 93.1
Zinc (Zn)Zn 6.0 to 7.0
Magnesium (Mg)Mg 0.6 to 0.8
Copper (Cu)Cu 0.35 to 0.65
Iron (Fe)Fe 0 to 0.5
Titanium (Ti)Ti 0 to 0.25
Silicon (Si)Si 0 to 0.15
Manganese (Mn)Mn 0 to 0.050
Residualsres. 0 to 0.15

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

ASTM B618: Standard Specification for Aluminum-Alloy Investment Castings

ASTM B26: Standard Specification for Aluminum-Alloy Sand Castings

Handbook of Aluminum Bonding Technology and Data, J. D. Minford, 1993

CRC Materials Science and Engineering Handbook, 4th ed., James F. Shackelford et al. (editors), 2015