H08 C11400 copper is C11400 copper in the H08 (spring) temper. It has the second highest strength and lowest ductility compared to the other variants of C11400 copper. The graph bars on the material properties cards below compare H08 C11400 copper to: wrought coppers (top), all copper alloys (middle), and the entire database (bottom). A full bar means this is the highest value in the relevant set. A half-full bar means it's 50% of the highest, and so on.

Mechanical Properties

Elastic (Young's, Tensile) Modulus

120 GPa 17 x 106 psi

Elongation at Break

2.8 %

Poisson's Ratio

0.34

Rockwell B Hardness

60

Rockwell F Hardness

94

Rockwell Superficial 30T Hardness

63

Shear Modulus

43 GPa 6.3 x 106 psi

Shear Strength

210 MPa 31 x 103 psi

Tensile Strength: Ultimate (UTS)

390 MPa 57 x 103 psi

Tensile Strength: Yield (Proof)

370 MPa 54 x 103 psi

Thermal Properties

Latent Heat of Fusion

210 J/g

Maximum Temperature: Mechanical

200 °C 390 °F

Melting Completion (Liquidus)

1080 °C 1980 °F

Melting Onset (Solidus)

1030 °C 1880 °F

Specific Heat Capacity

390 J/kg-K 0.092 BTU/lb-°F

Thermal Conductivity

390 W/m-K 220 BTU/h-ft-°F

Thermal Expansion

17 µm/m-K

Electrical Properties

Electrical Conductivity: Equal Volume

100 % IACS

Electrical Conductivity: Equal Weight (Specific)

100 % IACS

Otherwise Unclassified Properties

Base Metal Price

32 % relative

Density

9.0 g/cm3 560 lb/ft3

Embodied Carbon

2.6 kg CO2/kg material

Embodied Energy

42 MJ/kg 18 x 103 BTU/lb

Embodied Water

350 L/kg 41 gal/lb

Common Calculations

Resilience: Ultimate (Unit Rupture Work)

11 MJ/m3

Resilience: Unit (Modulus of Resilience)

600 kJ/m3

Stiffness to Weight: Axial

7.2 points

Stiffness to Weight: Bending

18 points

Strength to Weight: Axial

12 points

Strength to Weight: Bending

13 points

Thermal Diffusivity

110 mm2/s

Thermal Shock Resistance

14 points

Alloy Composition

Copper (Cu)Cu 99.84 to 99.966
Silver (Ag)Ag 0.034 to 0.060
Residualsres. 0 to 0.1

All values are % weight. Ranges represent what is permitted under applicable standards.

Followup Questions

Further Reading

ASTM B152: Standard Specification for Copper Sheet, Strip, Plate, and Rolled Bar